牌號(hào) 1.4542不銹鋼板和鋼帶
X5CrNiCuNb16-4
對(duì)應(yīng)標(biāo)準(zhǔn) NF EN 10088-2-2005
普通用途不銹鋼板和鋼帶的交貨技術(shù)條件
Part2:Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
歸類 沉淀硬化型不銹鋼
標(biāo)簽 特殊等級(jí)
X5CrNiCuNb16-4 化學(xué)元素成分含量(%)
成分 | C | Si | Mn | P | S ① | Cr | Ni | Cu | Mo | 更多 |
最小值 | - | - | - | - | - | 15 | 3 | 3 | - | Nb:5×C~0.45 |
最DA值 | 0.07 | 0.7 | 1.5 | 0.04 | 0.015 | 17 | 5 | 5 | 0.6 |
X5CrNiCuNb16-4 機(jī)械性能 | ||||
條件 | 熱處理或狀態(tài) | 抗拉強(qiáng)度 | 屈服點(diǎn) | 斷后伸長(zhǎng)率或延伸率 |
σb | σs | δ | ||
Mpa | Mpa | % | ||
冷軋帶鋼:T ≤ 8mm | +AT② | ≤1275 | - | ≥ 5① |
冷軋帶鋼:T ≤ 8mm | +P1300③ | ≥1300 | ≥1150 | ≥ 3① |
冷軋帶鋼:T ≤ 8mm | +P900③ | ≥900 | ≥700 | ≥ 6① |
熱軋中厚板:T ≤ 50mm | +P1070④ | 1070~1270 | ≥1000 | T< 3mm:≥ 8; |
T ≥ 3mm:≥ 10① | ||||
熱軋中厚板:T ≤ 50mm | +P950④ | 950~1150 | ≥800 | T < 3mm:≥ 10; |
T ≥ 3mm:≥ 12① | ||||
熱軋中厚板:T ≤ 50mm | +P850④ | 850~1050 | ≥600 | T < 3mm:≥ 12; |
T ≥ 3mm:≥ 14① | ||||
熱軋中厚板:T ≤ 50mm | +SR630⑤ | ≤1050 | - | - |
◎ T-厚度;l-縱向; t-橫向
◎ +A=軟化退火;+QT=淬火及回火;+P=沉淀硬化;+AT=固溶退火;+SR=消除應(yīng)力
① T<3mm時(shí)適用于標(biāo)距為80mm、寬度為20mm的試件。也可以使用標(biāo)距為50mm、寬度為12.5mm的試件。T ≥3mm時(shí)適用于標(biāo)距為5.65√S的試件。
② 交付條件。
③ 適用條件;可商定其他沉淀硬化溫度。
④ 如果在最終熱處理?xiàng)l件下訂購。